Plymouth Arrow hood

MP&C

Member
One of my former classmates from high school caught up with me a few months back, and had some work he wanted done on a hood for his Tubbed V8 Plymouth Arrow. Still has the same car from HS almost 4 decades later.. He said he wanted a more professional job over what was done back then..


HLgR4a7.jpg



He had bought an NOS hood for it some years back, so at least he has something solid to work with.. He said the metal flopped a bit around the opening he cut, so I thought we'd add a wire edge around the opening and make some new bracing on the underside while we were at it. Here's the phenolic dies made for the Lennox to form the new bracing..


xkWYSWL.jpg



Here's a test sample run...




...and a test fit


Kv2aRgu.jpg



Next, the bracing we wanted to install needed to go around the bigass hole, and some of the existing brace needed removing.


H85pPhz.jpg



9UR9mmH.jpg



Our new brace designed to go around the hole... cut in the flat and run through our dies..


Miq5USw.jpg



PqLFnTi.jpg



hBlrl8G.jpg



And here's about where it will sit....


lOxzwUp.jpg
 
Rather than screw up one of the last remaining NOS Plymouth Arrow hoods in existence, let's do a test sample first.. To strengthen the opening, we'll add a 1/8 wire edge protruding upward, which will also help to keep things out.....somewhat. Here's our new dies for the 1/8 wire... This is the "inlet" side...


F9YUtEI.jpg



Side view shows the ramps that will add the joggle


4eWKQCX.jpg



We're using a 22 x 22 piece of 19 gauge for our sample, and folding a 5/16 flange, which needs a bit of stretching to keep things flat. so a rounded hammer on the top of the stump adds a bit of stretch, then a linear stretch hammer and dolly to stretch further and fold things over..


ABicjt5.jpg



with the flange folded, the sample is run through our dies to form the joggle


ib2FRbD.jpg



1/8 stainless is rolled in our tubing bender/straightener, sized, and TIG welded to form a continuous ring. Then it gets laid in the channel and the flange staked over in various spots to hold it in place using the linear stretch hammer..


FP6hbJd.jpg



Hammering process to fold the flange over. Linear stretch hammer used to add a bit more stretch and to minimize marks left behind..




Finished sample...


PgRmIYC.jpg



….and checked to the brace


E77l9RW.jpg
 
Thanks!

With the practice behind us, lets see what we can do to this hood. The outer circle is the mark for our fold, or opening size. The inner circle is the cut for our flange that will wrap around the 1/8 wire..


LFdradY.jpg



Getting our tin snips started...


3BwHpyh.jpg



Hole cut with no filing, no sanding, and absolutely no metal "splinters".


soMuJt1.jpg



If you have issues with tin snips AT ALL, I recommend Bill Gibson's tin snip video... One of the best training/refresher videos on tin snips..




Next, on to the underside. We have four places where these areas of the old structure was cut out that need to go. Opening the hood to see these remnants would just kill the look, so let's see if we can mimic a factory look here.


R9Xb2Hp.jpg



A piece of 16 gauge was used as a heat shield and using the Meco torch and the barrel end hammer, reshaped the offset back to match the adjacent contour...


M6M8AXY.jpg



jV6MLDt.jpg



That'll do pig, that'll do.


9jl2RlG.jpg
 
With the hole cut now we need to fold a flange to wrap around the 1/8 wire. The linear stretch hammer and a heel dolly is used to stretch the flange that will be folded down, then a tipping tool takes the flange down about halfway. Then I needed to get in the thick of things, further stretching and hammering over to a 90* flange, all while checking the crown around the hole to ensure consistent stretch of the flange.


EBR5M2P.jpg



RoHIf8x.jpg



Once the flange is folded, the Lennox is used to add the joggle for our wired edge..




Bottom side....


qRnnpVz.jpg



bkhduMx.jpg



Top side....


1oaVHCh.jpg



h6S8hJ4.jpg



Our 1/8 stainless wire "ring" was formed using our tubing roller, the tool shown here in the vise when we were bending fuel line a few months back....


6w1XB1Y.jpg



The ring was then sized to fit, ends TIG welded together, filed, and media blasted for paint adhesion. The channel and surrounding area was abraded with some 120 grit and some SPI epoxy brushed into the channel. The wire gets laid into the channel and another brush coat on any bare spots. Then the flange is staked down using the linear stretch hammer to hold the wire in position...


hDZ9Ipm.jpg



Then the flange is hammered over as we did previously with our test sample.


jVZxvHv.jpg



After our initial coat of primer had dried, we brushed around the perimeter to seal the wire and flange.


LvacZsV.jpg
 
Excellent work MPC! I absolutely enjoy watching proficient quality metal work, and the order of operations. Thanks for the lessons too! Great clip on snips.
 
MPC,
what product do you use between the bracing and the hood skin? I see oem uses some sort of adhesive compound.
 
I haven’t gotten that far yet. I’m thinking of using some blobs of w/s setting compound. Any thoughts on that guys?
 
That commercial reminds me of the customized Ford denim van that I believe Hot Rod magazine gave away in a contest. if memory is correct I believe it was 1976. Interesting times they were.
 
Thanks Barry!

Looking at the bottom side of the hood, all of the structure uses a radius where the parts intersect, so we may as well follow suit.. Holes were cut in some 19 Gauge and corners cut out..

gpriIvL.jpg


Corners TIG welded and welds dressed..

iQ2x6KP.jpg


The area our brace will cover is abraded so we can get it covered with epoxy primer before installing the brace.

UhSBJP6.jpg


Brace is media blasted to prep for epoxy primer, and test fit to the hood.. Once the epoxy sets up a couple days we'll get the brace welded in..

OMikkMm.jpg


RT66GZG.jpg


t78EjWr.jpg


dZQINGe.jpg


Here are some older pictures of the car just to show what we're working on...

Uzypxx7.jpg


D4PXHdN.jpg


ZVsGPL8.jpg
 
I learned so much when I watched that video the first time (namely what I was doing wrong....) and it seemed a perfect place to slip it in. Glad it helped!


Prior to welding the brace in, we used some 3M NVH dampening material and added a few dabs on the inner hood skin where the brace's flanges would rest (Thanks to Chris Hamilton for the recommendation).

YlZLdGW.jpg



16 gauge cold rolled steel was used under the brace as a heat block for welding. The brace Is clamped, then tacked in place using the TIG.


yPpiwly.jpg



Uw5aIvo.jpg



TIG welded in short beads and checked the outside hood skin for heat, let cool and continued in that fashion.


Qg7brw9.jpg



Welds on the flat area of the flanges were dressed smooth. Remaining portion of the weld will likely be covered in a slight amount of filler to mimic the radius elsewhere under the hood.


RSuExl0.jpg



7icWYe6.jpg



Video of underside:





Topside with some epoxy on the bare parts....


Ag2fyYv.jpg
 
Last edited:
Back